Featured Stories
-
Back to the Beach: Global Pouch Forum 2024
The Global Pouch Forum1, produced by Packaging Strategies2, now in its 27th year, is the longest-running flexible packaging event in the... -
Innovation in Extrusion Barriers Can Reduce Brand Owners’ Dependence on Plastic
According to the most recent statistics from the Environmental Protection Agency1, in 2018 the U.S. produced 35 million tons of plastics, while... -
Tension: The First Thing We Must Get Right
Web tension is arguably the most important parameter for any web process. Tension is the first thing we must get right.
News | New Products
-
ProMach’s ID Technology Acquires Etiflex, a Leading Producer of Pressure-Sensitive Labels, Tickets, and RFID Labels in Mexico
ProMach, a worldwide leader in processing and packaging machinery and related solutions, announced today that it has acquired Etiflex
-
Re S.p.A. Celebrates 50 Years of Innovation at Drupa
Re S.p.A., an innovative leader in the printing and packaging industry, is excited to announce its participation in the next edition of Drupa
-
Sandon Global to bring anilox excellence and technical know-how to drupa 2024
Sandon Global, the British anilox manufacturer and drupa 2024 exhibitor, is poised to showcase its extensive technical expertise in flexographic printing
-
TIPA Compostable Packaging Appoints John Wilson as Commercial Director for North America
Packaging and sustainability industry veteran joins TIPA, to drive US adoption of compostable packaging to curb plastic waste
-
INX promotes three to Vice President positions
The Board of Directors at INX International Ink Co. have approved the promotions of three key executive managers to vice president positions.
-
Rogelio Barba Villagran Named Business Development Director for AGH Labels North America
AGH Labels, headquartered in Leon, Mexico, is excited to announce long-time executive, Rogelio Barba Villagran, as its business development director for AGH Labels North America.
-
Hong Kong PrintPack Fairs Open in April
Jointly organized by the Hong Kong Trade Development Council and CIEC Exhibition Company (HK) Limited, the two PrintPack Fairs will be April 27-30, 2024 at AsiaWorld-Expo
Expert Advice
Can This Lamination Be Saved?
- Published: August 31, 2004, By Timothy J. Walker TJWalker & Assoc. Inc.
Delaminating — undesired separation within a multilayer product — is a major problem for many converters.
Laminate products are a marriage of two or more layers with combined properties not found in any individual layer. Delamination is the breakup of this marriage when outside forces exceed the ties that bind.
If coatings are counted as layers, almost all converted products could be considered laminates. As I refer to laminates in this column, I'm generally thinking about substrate layers and stiffer and thicker coated layers. For a laminate to work, we usually want the layers to stay together. But, look out! There are forces at work to undermine the marriage of your laminate layers.
Products with intentionally low laminate bonds will be more susceptible to unintended delamination. For example, label stock will need more care in processing to avoid an early breakup, since ease of delamination is a desired end-customer feature.
Many laminating processes create a product with weak initial bond strength, sometimes called “green strength.” Often a laminate bond involves curing, whether chemical or added by outside energy, developing a stronger bond over time. Therefore, the most important period to deter delamination is just after initial bonding.
In web handling, the excitement usually happens at the web-roller interface. Going around a roller should be an elastic experience. When your flat web is forced around the cylinder of a roller, the curved shape will impose tensile and compressive stresses on the outer and inner surfaces, respectively. These stresses are proportional to the product thickness divided by the roller radius.
Many web processes have specifications for minimum bending radius or roller diameter, aimed at avoiding curvature-induced stresses beyond a product's elastic limits. However, for laminates, you may need to set a larger minimum roller diameter, since the forces to cause delamination may be well short of elastic limits.
As a laminate wraps around a roller, the layers respond with a through-thickness stress and strain change. At the interface, the inside is attempting to elongate while the outside layer is trying to contract. This mechanical opposition creates a shear force at the bond point. If the shear load is greater than the laminate bond, the laminate will split apart.
When two webs are transported over the same roller, there is a natural tendency for the top web to have greater velocity. Assuming no slip, the average web speed going around a roller is determined by the roller revolutions per minute and the circumference of the center line of the web. When two webs wrap a roller together, the small difference in the centerline circumference will create a significant long-term length variation.
For example, two 1-mil webs will have a 1-mil radial centerline difference and a 0.006-in. feed length variation per roller revolution. This doesn't seem like much, but at 100 fpm on a 4-in.-dia roller, this adds up to 0.6 in./min of extra material in the bottom web.
When two webs have low or no bond, this extra material will pile up on the floor, wrap on the roller, or fold over in a crossweb wrinkle — all undesired outcomes. If a laminate has high bond strength, the two layers will act as one, the top web will stretch, the bottom will contract, and there will be no delamination or feed rate variations.
Here are four tips to avoid roller curvature and feed rate-induced delamination:
- Move to large-diameter rollers. The curvature-induced delaminating stresses go down inversely proportional to diameter.
- Avoid rollers until bond strength increases. If you postpone roller curvature until green strength goes up, you may avoid delamination.
- Increase tension. The pressure created by the outer web's tension will add to the laminate bond force, increasing the resistance to delaminate.
- Use lateral or low-angle spiral-ridged rollers. Roller ridges may not prevent delamination, but they can burp through small feed variations, preventing the catastrophe of web wrinkling or wrapping rollers.